超超临界机组用P92钢高温服役8000h后显微组织与韧性Microstructure and toughness of steel P92 used in ultra supercritical unit after 8000h service at high temperature
刘睿,邹勇,张忠文,杜宝帅
摘要(Abstract):
利用光学显微镜、X射线衍射仪、扫描电镜及能谱仪和冲击试验研究了运行了8000 h的1000 MW超超临界机组主蒸汽管道P92钢的显微组织和韧性。结果表明,主蒸汽管道P92钢在600℃服役8000 h后,显微组织呈现大量析出相分布于马氏体基体之上的形貌,析出相除了供货状态(正火+高温回火)存在的MX相以及M23C6相之外,还有时效后在原奥氏体晶界和马氏体板条界处产生的Laves相;运行8000 h后,P92钢的韧性明显地下降,这主要与Laves相的析出和粗化有关。
关键词(KeyWords): 超超临界机组;P92钢;显微组织;韧性;laves相
基金项目(Foundation): 山东省科技攻关项目(2008GG30001017)
作者(Author): 刘睿,邹勇,张忠文,杜宝帅
DOI: 10.13289/j.issn.1009-6264.2014.09.023
参考文献(References):
- [1]唐飞,董斌,赵敏.超超临界机组在我国的发展及应用[J].电力建设,2010,31(1):80-82.TANG Fei,DONG Bin,ZHAO Min.USC unit development and application in China[J].Electric Power Construction,2010,31(1):80-82.
- [2]徐通模,袁益超,陈干锦,等.超大容量超超临界锅炉的发展趋势[J].动力工程,2003,23(3):2363-2369.XU Tong-mo,YUAN Yi-chao,CHEN Gan-jin,et al.Developmental trend of super-large capacity and ultra supercritical boilers[J].Power Engineering,2003,23(3):2363-2369.
- [3]杨富,章应霖,任永宁,等.新型耐热钢焊接[M].北京:中国电力出版社,2006.
- [4]Lomozik M,Zeman M,Brózda J.Modern martensitic steels for power industry[J].Archives of Civil and Mechanical Engineering,2012,12(1):49-59.
- [5]Vaillant J C,Vandenberghe B,Hahn B,et al.T/P23,24,911 and 92:New grades for advanced coal-fired power plants—Properties and experience[J].International Journal of Pressure Vessels and Piping,2008,85(1):38-46.
- [6]Kim B,Jeong C,Lim B.Creep behavior and microstructural damage of martensitic P92 steel weldment[J].Materials Science and Engineering A,2008,483:544-546.
- [7]彭志方,蔡黎胜,彭芳芳,等.P92钢625℃持久性能分段特征与各段中M23C6及Laves相相参数的定量变化研究[J].金属学报,2010,46(4):429-434.PENG Zhi-fang,CAI Li-sheng,PENG Fang-fang,et al.Study on the multi-segment feature of 625℃creep-rupture property and the quatitative change of phase parameters of M23C6and Laves phases in each segment of P92 steel[J].Acat Metallurgica Sinica,2010,46(4):429-434.
- [8]王学,潘乾刚,陈方玉,等.P92钢高温蠕变损伤分析[J].材料热处理学报,2010,31(2):65-69.WANG Xue,PAN Qian-gang,CHEN Fang-yu,et al.Analysis of creep damage at elevated temperature in a P92 steel[J].Transactions of Materials and Heat Treatment,2010,31(2):65-69.
- [9]Pétry C,Lindet G.Modelling creep behaviour and failure of 9Cr-0.5Mo-1.8W-VNb steel[J].International Journal of Pressure Vessels and Piping,2009,86(8):486-494.
- [10]殷尊,蔡晖,刘鸿国.1000 MW超超临界机组用P92耐热钢高温服役后的性能[J].材料热处理学报,2012,33(11):105-110.YIN Zun,CAI Hui,LIU Hong-guo.Performance of heat-resistant steel P92 used in 1000 MW ultra supercritical unit after long-term service at high temperature[J].Transactions of Materials and Heat Treatment,2012,33(11):105-110.
- [11]李玲霞,刘正东,赵晓丽,等.P92耐热钢物理化学相分析[J].冶金分析,2013,33(2):1-7.LI Ling-xia,LIU Zheng-dong,ZHAO Xiao-1i,et al.Physicochemical phase analysis of heat resistant steel P92[J].Metallurgical Analysis,2013,33(2):1-7.
- [12]Abe F.Precipitate design for creep strengthening of 9%Cr tempered martensitic steel for ultra-supercritical power plants[J].Science and Technology of Advanced Materials,2008,9(1):13002-13016.
- [13]Guo X,Gong J,Jiang Y,et al.The influence of long-term aging on microstructures and static mechanical properties of P92 steel at room temperature[J].Materials Science and Engineering A,2013,564:199-205.
- [14]Httestrand M,Andren H-O.Evaluation of particle size distributions of precipitates in a 9%chromium steel using energy filtered transmission electron microscopy[J].Micron,2001,32(8):789-797.
- [15]姜筠,朱丽慧,王延峰.P92钢高温持久强度试验后组织变化对性能的影响[J].动力工程学报,2012,32(11):898-902.JIANG Jun,ZHU Li-hui,WANG Yan-feng.Effect of microstructure evolution on property of P92 steel during high-temperature creep-rupture tests[J].Journal of Chinese Society of Power Engineering,2012,32(11):898-902.
- [16]Panait C G,Zielińska-Lipiec A,Koziel T,et al.Evolution of dislocation density,size of subgrains and MX-type precipitates in a P91 steel during creep and during thermal ageing at 600℃for more than 100,000 h[J].Materials Science and Engineering A,2010,527(16):4062-4069.
- [17]Korcakova L,Hald J,Somers M A.Quantification of Laves phase particle size in9CrW steel[J].Materials Characterization,2001,47(2):111-117.
- [18]Prat O,Garcia J,Rojas D,et al.The role of Laves phase on microstructure evolution and creep strength of novel 9%Cr heat resistant steels[J].Intermetallics,2013,32:362-372.
- [19]郝曼曼,彭碧草,王起江,等.T92钢在蠕变过程中Laves相的析出与熟化行为[J].机械工程材料,2011,35(10):32-35.HAO Man-man,PENG Bi-cao,WANG Qi-jiang,et al.Precipitation and coarsening of Laves phases in T92 steels in the process of creep[J].Materials for Mechanical Engineering,2011,35(10):32-35.
- [20]石如星,刘正东.P92钢中Laves相强化作用的研究[J].物理测试,2011(4):5-9.SHI Ru-xing,LIU Zheng-dong.Study on strengthening behavior of Laves phase in P92 heat-resistant steel[J].Physics Examination and Testing,2011(4):5-9.
- [21]Srinivas Prasad B S,Rajkumar V B,Hari Kumar K C.Numerical simulation of precipitate evolution in ferritic-martensitic power plant steels[J].Calphad,2012,36:1-7.
- [22]张红军,周荣灿,范长信.Laves相对P92钢冲击韧性影响的试验研究[J].动力工程学报,2012,32(1):84-88.ZHANG Hong-jun,ZHOU Rong-can,FAN Chang-xin.Influence of Laves phase on impact toughness of P92 steel[J].Journal of Chinese Society of Power Engineering,2012,32(1):84-88.
- [23]Li S,Eliniyaz Z,Sun F,et al.Effect of thermo-mechanical treatment on microstructure and mechanical properties of P92 heat resistant steel[J].Materials Science and Engineering A,2013,559:882-888.
- [24]何肇基.金属力学性能[M].北京:冶金工业出版社,1982.
文章评论(Comment):
|
||||||||||||||||||
|
||||||||||||||||||